化学学报 ›› 2023, Vol. 81 ›› Issue (6): 565-571.DOI: 10.6023/A23040163 上一篇    下一篇

研究通讯

基于环烷烃/乙醇混合碳源高性能碳纳米管纤维的连续化制备

赵天成, 蒋鸿宇, 张琨, 徐一帆, 康欣悦, 胥鉴宸, 周旭峰, 陈培宁*(), 彭慧胜*()   

  1. 聚合物分子工程国家重点实验室 复旦大学高分子科学系 先进材料实验室 上海 200438
  • 投稿日期:2023-04-25 发布日期:2023-05-31
  • 基金资助:
    国家自然科学基金(T2222005); 国家自然科学基金(22175042); 上海市科委(21511104900); 上海市科委(20JC1414902)

Continuous Preparation of High-performing Carbon Nanotube Fibers Based on Cycloalkane/ethanol Mixing Carbon Source

Tiancheng Zhao, Hongyu Jiang, Kun Zhang, Yifan Xu, Xinyue Kang, Jiancheng Xu, Xufeng Zhou, Peining Chen(), Huisheng Peng()   

  1. State Key Laboratory of Molecular Engineering of Polymers, Department of Macromolecular Science, Laboratory of Advanced Materials, Fudan University, Shanghai 200438
  • Received:2023-04-25 Published:2023-05-31
  • Contact: *E-mail: peiningc@fudan.edu.cn, penghs@fudan.edu.cn
  • Supported by:
    National Natural Science Foundation of China(T2222005); National Natural Science Foundation of China(22175042); Science and Technology Commission of Shanghai Municipality(21511104900); Science and Technology Commission of Shanghai Municipality(20JC1414902)

利用化学气相沉积和干法纺丝方法可以制备得到碳纳米管纤维, 但受限于反应碳源较为单一, 目前纤维的力学和电学性能还难以有效满足实际应用需求, 如何实现高性能碳纳米管纤维的连续制备, 仍是本领域一个重要挑战. 本研究通过设计十氢萘/乙醇新型二元混合碳源, 重点调控环烷烃/乙醇的组分比例, 实现了高性能碳纳米管纤维的连续化制备, 收集速率达到220 m/h. 相比于已报道的由单一乙醇碳源制备的碳纳米管纤维, 由混合碳源制备的碳纳米管纤维拉伸断裂强度(750 MPa)提升了1倍以上, 力学性能在弯折百万次后仍保持稳定; 电导率(4.8×103 S/cm)提升4倍以上, 可有效满足纤维储能器件应用需求, 所构建的纤维状锂-二氧化碳电池显示良好电化学性能.

关键词: 碳纳米管纤维, 化学气相沉积, 浮动催化剂, 连续制备, 混合碳源

Due to the excellent physical and chemical properties, carbon nanotubes show broad applications in a variety of fields such as composite materials, catalysis, energy, medicine and sensor. However, at present, the carbon nanotubes are mainly practically used in the form of powders. Carbon nanotube fibers can be prepared by the methods of chemical vapor deposition and/or dry spinning. However, the carbon source used in previous study mainly has single component, making the mechanical and electrical properties of carbon nanotube fibers still difficult to effectively meet the practical application requirements. It remains challenging to realize continuous preparation of high-performance carbon nanotube fibers. In this work, a new cycloalkane/ethanol mixing carbon source was designed to obviously promote the continuous growth process and properties of carbon nanotube fibers. After carefully optimizing the component ratio of decahydronaphthalene/ethanol in the precursor solution, and systematically optimizing reaction conditions such as catalyst content (ferrocene and thiophene), injection rate of the precursor solution, and the flow rate of carrier gas (argon and hydrogen), the continuous preparation of high-performance carbon nanotube fibers was realized. When the mass ratio of decahydronaphthalene to ethanol carbon source in precursor solution is 3∶7, the high-performance carbon nanotube fibers can be continuously produced for a long time with a collection rate of 220 m/h. It shows improved mechanical and electrical properties compared with the carbon nanotube fiber prepared by using single ethanol carbon source. For instance, the tensile strength of carbon nanotube fiber is increased by more than 1 time (750 MPa). The carbon nanotube fiber has good flexibility and can shows stable mechanical properties after millions of bending cycles. The conductivity is increased by more than 4 times (4.8×103 S/cm), which can effectively meet the application requirements of fiber energy-storing devices. The application of carbon nanotube fibers in a fiber-shaped lithium-carbon dioxide battery is demonstrated with good electrochemical performance.

Key words: carbon nanotube fiber, chemical vapor deposition, floating catalyst, continuous preparation, mixing carbon source